调质贝氏体鱼尾板
化学成分
C:0.15% Mn:1.026% Si :0.576% P<0.006% S<0.007%
Cr: 0.299% V :0.028% Nb:0.04-0.07% Cu :0.121% Ni: 0.030%
力学性能
b:966.3MPa s:722.3MPa :18.7% Ak 60.7J 冷弯60
3、美国XY-30低温高强度鱼尾板
化学成分
C:0.33% Mn :1.49% Si:0.32% P:0.016% S :0.017% C r:0.07 %
V:0.12%Nb: 0.04% Cu :0.18% Ni:0.05% Mo:0.19% Ti:0.001%
未做热处理机械性能
b900 MPa s 780MPa 17% 40% HB245-276 Ak38.5J-30℃
冷弯30完好
4、DY-30鱼尾板
化学成分
C:0.20-0.38